EDM hole drilling
EDM drilling — hole popping — burns a hole with a rotating tubular electrode in a dielectric bath. It has no drill to break, no cutting force and no work hardening, and it reaches depth-to-diameter ratios that no twist drill can.
Send a drawingHow it differs from drilling
A twist drill cuts with a sharp edge and needs the material to be softer than the drill. EDM drilling erodes with sparks between a tubular electrode and the workpiece, so material hardness is almost irrelevant and there is no mechanical force.
The electrode is a brass or copper tube, typically 0.3-3 mm, and the dielectric is flushed through the centre. The hole is slightly larger than the tube by the spark gap, and the edge has a small recast layer rather than a burr.
| Aspect | Twist drilling | EDM drilling |
|---|---|---|
| Material hardness | Must be softer than drill | Any conductive material |
| Cutting force | Significant | None |
| Depth / diameter | Up to 10:1 | Up to 100:1 |
| Hole size | 0.5 mm and up, easily | 0.3-3 mm typical |
| Burr | Yes | Minimal, recast layer instead |
| Speed | Fast | Slow |
Depth-to-diameter is the reason it exists
At 30:1 a twist drill wanders, the chip packs and the drill breaks. EDM drilling reaches 50:1 and beyond routinely, because there is no chip to evacuate in the mechanical sense and no bending force on the tool.
That is how cooling holes in turbine blades, injector nozzle orifices and deep lubrication passages in hardened dies are made. The hole is straight because nothing pushes the electrode sideways.
| L/D | Twist drill | EDM drilling |
|---|---|---|
| Up to 5:1 | Routine | Possible but slow |
| 5-10:1 | Through coolant, peck | Comfortable |
| 10-30:1 | Gun drilling | Routine |
| 30-50:1 | Difficult | Routine |
| Over 50:1 | Specialist | Specialist |
Recast layer and what to do about it
Every EDM process leaves a recast layer — a thin skin of re-solidified metal, plus a heat-affected zone behind it. On a cooling hole it is usually acceptable; on a fatigue-critical hole it is a crack initiation site.
The layer is 5-30 µm depending on the power. It can be removed by a low-energy finishing pass, by abrasive flow, or by electropolishing, and the drawing should say whether it must be removed.
| Requirement | Recast allowed | Action |
|---|---|---|
| Cooling hole | Yes | None |
| Hydraulic passage | Minimal | Finishing pass |
| Fatigue-critical | No | Abrasive flow or polish |
| Medical | No | Electropolish |
| Injection nozzle | Depends on flow | Finishing pass |
Where it is used here
Hardened dies and punches that need a lubrication hole after heat treatment, deep passages in stainless and titanium parts, and any small hole in material that would break a drill.
It is a partner process. The drawing review decides whether the hole is better drilled before hardening — usually cheaper — or EDM drilled after.
Tolerance, taper and what to specify
Position is typically 0.02-0.05 mm, diameter 0.02-0.05 mm, and there is a small taper over the depth because the electrode wears. On a deep hole that taper is measurable and should be specified as acceptable or not.
Specify the diameter, the depth, the position and whether the recast layer matters. Those four decide whether it is a $5 hole or a $50 hole.
| Feature | Typical | Note |
|---|---|---|
| Hole diameter | 0.3-3 mm | Smaller needs micro EDM |
| Diameter tolerance | ±0.02-0.05 mm | Electrode wear dependent |
| Position | ±0.02-0.05 mm | Per the drawing datum |
| Taper | 0.02-0.1 mm over depth | Specify if critical |
| Recast | 5-30 µm | Removable |
Electrode types and wear
The electrode is a brass or copper tube, and it wears as it burns. Brass is cheap and wears faster; copper wears more slowly and holds diameter better on deep holes. Some electrodes are coated to reduce side wear.
Wear shows up as a hole that is smaller at the bottom than the top, and as a diameter that drifts over a long run. The usual compensation is to start with a slightly larger tube, or to use a fresh electrode for the finishing pass on a critical hole.
| Electrode | Wear | Cost | Use |
|---|---|---|---|
| Brass tube | Higher | Low | General holes |
| Copper tube | Lower | Medium | Deep, accurate |
| Coated copper | Lowest | Higher | Production, tight diameter |
| Solid electrode | Very low | High | Shaped or blind features |
Dielectric and flushing
The dielectric does two jobs: it insulates until the spark jumps, and it flushes the eroded debris out of the hole. Flushing through the electrode centre is what makes deep holes possible.
Poor flushing shows up as a slow burn, a tapered hole and occasional short circuits — the electrode backs up, the burn stalls, the hole takes twice as long. On deep holes, through-flushing at pressure is not optional.
| Flushing | Depth capability | Symptom if poor |
|---|---|---|
| Through the electrode | Best, 50:1+ | — |
| Side flushing | Moderate | Taper, slow |
| Immersion only | Shallow | Stalling, short circuits |
| Suction | Specific cases | Debris build-up |
Angled, curved and shaped holes
EDM drilling can start on an angled surface and can drill at an angle, which is how cooling holes in turbine blades are made — they enter at a shallow angle to the surface and follow a defined path.
A shaped hole needs a shaped electrode: a square, a slot or a profiled tube. The same electrode can only make one shape, so a shaped hole has a tooling cost that a round hole does not.
Curved holes need a curved electrode path, which is a specialist machine. It is quoted case by case and is not a standard capability.
| Hole type | Electrode | Note |
|---|---|---|
| Round, straight | Tube | Standard |
| Angled entry | Tube, angled head | Turbine cooling |
| Shaped (square, slot) | Profiled electrode | Tooling cost |
| Curved | Specialist path | Case by case |
| Blind | Solid or tube | Depth control |
Cost per hole and how to reduce it
Cost is driven by depth, diameter and the number of holes. A shallow 3 mm hole is seconds; a 50:1 hole is minutes, and the electrode wears out doing it.
The biggest lever is doing the hole before hardening when the geometry allows — a drilled hole before heat treatment is a fraction of the EDM cost. The second is grouping: many holes in one setup share the positioning time.
The third is asking whether the hole needs the full depth. A lubrication passage that only needs to reach an intersecting bore can often be shorter than the drawing suggests.
| Factor | Effect on cost | Lever |
|---|---|---|
| Depth / diameter | Dominant | Drill before hardening |
| Hole count | Linear plus setup | Group in one setup |
| Diameter | Smaller costs more | Specify the largest that works |
| Tolerance | Moderate | Relax if functional |
| Recast removal | Adds a step | Specify only where needed |
Prep, clean-up and the hand-off
The hole comes off the machine with a recast edge and often a small burr at the entry. On a part that will be inspected, that edge is the first thing the inspector sees, and on a fluid part it is the first thing that affects flow.
Deburring a 0.5 mm hole is not a file job. It is a light abrasive flow or an electropolish, and it should be quoted with the hole rather than discovered afterwards — because the cost of cleaning up a hundred small holes can exceed the cost of drilling them.
| Requirement | Clean-up | Note |
|---|---|---|
| Cooling hole | None | Recast accepted |
| Fluid passage | Abrasive flow | Removes recast and burr |
| Visible hole | Light deburr | Appearance |
| Medical | Electropolish | Cleanability |
FAQ
- Can EDM drill hardened steel?
- Yes, hardness is almost irrelevant. That is the main reason it exists.
- How deep can it go?
- Up to 50:1 or more, against about 10:1 for a twist drill.
- Is there a burr?
- Almost none — a small recast layer instead, which can be removed.
- Is it faster than drilling?
- No. It is slower, and it is used where drilling cannot reach or would break.
- What is the smallest hole?
- About 0.3 mm with standard EDM drilling; smaller with micro EDM.
- Does it need a starter hole?
- No, it starts from the surface.
- Can it drill at an angle?
- Yes, with an angled electrode or a tilting head, for angled cooling holes.
- Does it affect the heat treatment?
- The recast layer is local. Below it, the bulk hardness is unchanged.
Have a drawing to review?
Send the model, the revision and the quantity. You get a written review of the open items with the price.