Process

Sheet metal bending

A bend is not a line on a flat pattern. The metal stretches on the outside and compresses on the inside, and the flat length has to account for that — which is why the same part bends short if the shop uses the wrong K-factor.

Send a drawing

Bend allowance is the whole calculation

When a sheet is bent, the neutral axis stays the same length while the outer surface stretches and the inner compresses. The flat pattern length is the sum of the straight sections plus the arc length at the neutral axis — that arc is the bend allowance.

Where the neutral axis sits is the K-factor, and it depends on the material, the bend radius and the method. For air bending it is typically 0.33-0.5 of the thickness. Use the wrong K-factor and every bend in the part is off by a fraction of a millimetre, which accumulates across a sequence of bends.

ParameterTypical valueDepends on
K-factor0.33-0.5Material, radius, method
Bend allowanceArc at neutral axisK-factor, angle, radius
Bend deductionUsed by most CADDerived from allowance
Inside radius≥ thickness (steel)Material and temper

Minimum bend radius

Bending tighter than the material allows cracks the outside of the bend. The limit is expressed as a multiple of thickness, and it is different for each alloy and temper.

For mild steel it is roughly one thickness; for aluminum it is 1-2 thicknesses depending on temper (5052-H32 bends better than 6061-T6); for stainless 304 it is about one thickness in the annealed condition and two or more work-hardened.

MaterialMin radius (× thickness)Note
Mild steel1.0Forgiving
Stainless 304 annealed1.0Work hardens in the bend
Aluminum 5052-H321.0-1.5Good forming alloy
Aluminum 6061-T62.0-3.0Cracks easily, avoid
Aluminum 7075-T63.0+Not a forming alloy

Springback and how it is handled

Every bend springs back when the punch is released, because the outer surface was stretched elastically as well as plastically. The amount depends on the material’s yield strength and the radius-to-thickness ratio.

The press brake compensates by overbending — driving the punch slightly past the target angle. On a controlled machine that is a programmed offset; on an old machine it is the operator’s experience, and it varies by material batch.

MaterialSpringbackCompensation
Mild steel1-3°Small overbend
Stainless3-8°Significant overbend
Aluminum2-5°Moderate
High strength steel8-15°Large, may need coining

Design rules that avoid rework

A hole too close to a bend distorts, because the material flows toward the bend line. The usual rule is a hole at least 2.5 thicknesses plus the bend radius from the bend line.

A bend needs relief at its ends if the flange is short or the part has a corner, or the material tears. And a bend line that crosses a previously bent region cannot be formed in one hit — it needs a different sequence or a different design.

FeatureRuleConsequence
Hole to bend≥ 2.5t + RHole distorts
Bend reliefAt each endTearing
Flange length≥ 4t or the die widthCannot form
Bend sequencePlan the orderCollision with the punch

What a press brake holds

Angle is held to about ±1°, bend position to ±0.2 mm, and hole position on a laser-cut blank to ±0.1 mm. Those are the numbers to design to.

If the part needs a 0.05 mm relationship between a machined face and a bend, the bend is the wrong feature — machine it instead, or weld a machined pad into the bent part.

FeatureToleranceNote
Bend angle±1°Springback dependent
Bend position±0.2 mmFlat pattern dependent
Laser-cut hole±0.1 mmBefore bending
Hole to bend±0.3 mmHarder to hold
Overall flatnessDistorted by bendsNot a flat part

Tooling: the V-die decides the radius

In air bending the inside radius is not set by the punch nose — it is set by the die opening. A rule of thumb is that the inside radius is about one sixth of the V-die width, so an 8 mm V gives roughly a 1.3 mm radius.

That means the drawing’s radius and the shop’s die must agree. A drawing calling R1 on 3 mm steel, when the available die produces R1.5, will be bent to R1.5 or forced with a sharper punch that marks the inside of the bend.

Die width also sets the tonnage: a wider V needs less force per metre, so it is cheaper on the machine but gives a larger radius. The two are traded against each other on every job.

V-die widthInside radius (approx)TonnageUse
6 mm1.0 mmHighThin sheet
8 mm1.3 mmMediumGeneral 2-3 mm
12 mm2.0 mmLower3-5 mm
16 mm+2.7 mm+LowestThick plate

Tonnage, and why the machine matters

Bending force scales with thickness squared, with the bend length, and inversely with the die width. Doubling the thickness quadruples the tonnage for the same length and die — which is why thick parts need a big brake and thin parts do not.

Exceeding the tonnage does not fail gracefully: the punch or the die cracks, or the machine’s frame deflects and the bend is uneven along its length. A long bend on a small brake bows in the middle, and that shows up as a part that is not straight.

ThicknessLengthRelative tonnage
1 mm1 m1.0
2 mm1 m4.0
3 mm1 m9.0
2 mm2 m8.0

Bend sequence and collision

A part with several bends has an order. Bend the wrong one first and the flange collides with the punch on a later hit, and the part cannot be finished.

The usual rule is to bend the outermost features first and work inward, and to keep long flanges until later so the part is still flat enough to handle. On a complex bracket the sequence is planned before the flat pattern is released, not discovered at the machine.

SituationSequenceWhy
Two opposite flangesShort one firstAccess
Box with four sidesLong sides, then endsPunch clearance
Return flangeMain bend, then returnTooling access
Close bendsAlternate sidesDie collision

After bending: weld, finish and assembly

A bent part is usually welded, and welding distorts it. The sequence that works is bend, weld, then machine or finish the features that must stay true — not the other way round.

For a powder-coated part the weld has to be dressed before coating, and the part has to be clean. For an anodized part, note that anodizing does not hide weld discolouration; the weld is usually ground and blended first.

And a bent part is not flat. If a machined face is needed, it is machined after bending, or a separate machined pad is welded in — trying to hold flatness through a bend sequence does not work.

StepEffectOrder
BendDistorts flatnessFirst
WeldDistorts moreAfter bending
Machine facesRestores toleranceAfter welding
FinishCovers or revealsLast

What a bent part is not

A bent part is not a precision part. It is a near-net shape that is accurate in the flat and approximate in the third dimension, and the parts that need accuracy are machined afterwards.

That distinction decides which features belong on the bend drawing and which belong on a machining operation. A hole pattern that locates an assembly belongs in a machined plate; a hole that clears a cable can be laser cut before bending.

FAQ

Why is my bent part short?
The flat pattern used the wrong K-factor or bend deduction.
What is the minimum bend radius?
Roughly one thickness for mild steel and annealed stainless, more for harder alloys.
Why does the bend spring back?
Elastic recovery. The brake overbends to compensate, by 1-8° depending on material.
Can 6061-T6 be bent?
Poorly — it cracks at tight radii. 5052 is the forming alloy.
How far should a hole be from a bend?
At least 2.5 thicknesses plus the bend radius.
What tolerance does bending hold?
About ±1° on angle and ±0.2 mm on position.
Can you bend after machining?
Yes, but the bend will distort nearby machined features. Machine after bending where possible.
What is bend relief?
A notch at the end of a bend that stops the material tearing.