Bead blasting
Bead blasting is not cleaning. It is a controlled surface treatment that hides tool marks, sets the base for anodizing and changes the roughness — and the media, the pressure and the distance decide all three.
Send a drawingWhat blasting does to a surface
Glass bead peens the surface with round media, producing a uniform matte without cutting. Aluminum oxide is angular and cuts, producing a rougher, more aggressive finish. Ceramic bead sits between them and lasts longer.
The change is both topographical and mechanical: the surface is slightly work-hardened, and the peaks from machining are flattened and blended into a uniform texture.
| Media | Shape | Ra produced | Use |
|---|---|---|---|
| Glass bead 100-200 µm | Round | Ra 0.8-1.6 | Anodizing prep, matte |
| Glass bead 50-100 µm | Round | Ra 0.4-0.8 | Fine matte |
| Ceramic bead | Round, hard | Ra 0.4-0.8 | Longer media life |
| Aluminum oxide | Angular | Ra 1.6-3.2 | Rougher prep, paint key |
| Walnut shell | Soft | Minimal | Delicate parts, plastic |
| Dry ice | Sublimating | None | Cleaning only |
Why it goes before anodizing
Clear anodizing is transparent, so it shows every tool mark on the surface underneath. A bead blast gives a uniform matte that the oxide takes evenly, and the result reads as a deliberately finished surface rather than a machined one.
Coloured anodize hides more, but colour can still vary with surface roughness: a polished face takes dye darker than a blasted one, so mixed finishes on one part will not match.
Effect on dimensions and edges
Blasting removes a few microns — typically 2-5 µm — and rounds edges. On a tight tolerance it is negligible; on a sharp edge or a knife-edge feature it is significant.
It also closes very small features: a 0.2 mm hole can be partly masked by peening, and a fine thread can be affected. Mask them or accept the change.
| Feature | Effect | Action |
|---|---|---|
| Thickness | −2 to −5 µm | Negligible |
| Edge | Rounded | Specify if sharp is needed |
| Fine thread | Slightly affected | Mask or chase |
| Small hole under 0.5 mm | Can close partly | Mask |
| Ra | Set by media | Choose the media |
Masking and selective blasting
A part can be blasted on one face and left as-machined on another, which is common when the sealing face must stay smooth or the bore must keep its tolerance.
Masking is manual work and it is priced. On a complex part with many masked areas, the masking can cost more than the blasting — which is worth knowing before designing a face that is both cosmetic and precision.
| Area | Blast or mask | Why |
|---|---|---|
| Cosmetic face | Blast | Hides tool marks |
| Sealing face | Mask | Keeps Ra 1.6 |
| Precision bore | Mask | Keeps tolerance |
| Thread | Mask or chase | Protects the fit |
| Ground face | Mask | Protects flatness |
Control and uniformity
The variables are media size and condition, pressure, nozzle distance and angle, and dwell time. Change any one and the finish changes.
A shop that blasts by feel produces parts that differ between batches. A controlled process specifies the media, the pressure and the pass, and checks against a sample. On a visible part, the sample is the specification.
| Variable | Effect | Control |
|---|---|---|
| Media size | Roughness | Specify the grade |
| Media condition | Breakdown changes Ra | Replace on schedule |
| Pressure | Depth and rate | Set and record |
| Distance and angle | Uniformity | Fixture the nozzle |
| Dwell time | Depth of texture | Timed pass |
Bead blasting compared with the alternatives
Several processes produce a matte finish, and they are not interchangeable. Sandblasting uses silica sand, which is cheap and produces a good matte — and creates a respirable silica hazard that has largely driven it out of professional shops.
Vapor blasting (wet blasting) mixes abrasive with water, producing a finer, brighter, almost peened finish with no dust. Tumbling produces a matte with rounded edges and is uniform across a batch. Each has a place, and the choice changes both the look and the cost.
| Process | Finish | Edge | Note |
|---|---|---|---|
| Glass bead (dry) | Even matte | Slightly rounded | The anodizing prep standard |
| Aluminum oxide (dry) | Rougher matte | Rounded | Paint key |
| Vapor blasting (wet) | Fine, bright satin | Rounded, gentle | No dust, premium look |
| Sandblasting | Coarse matte | Rounded | Silica hazard |
| Vibratory tumbling | Uniform matte | Noticeably rounded | Bulk parts |
| Chemical etch | Uniform satin | Sharp, unchanged | No mechanical effect |
Blasting plastic and soft metal
Plastic and soft aluminum need low pressure and fine media, because the same blast that textures steel will erode or distort them. Walnut shell, fine glass bead and low pressure are the combination for plastics.
Thin aluminum panels are the other risk: peening puts the surface into compression, and on a thin section that is enough to bow the part. Support the panel from behind, blast both faces, or reduce the pressure until the movement is acceptable.
On plastic, blasting also changes the surface chemistry slightly — it raises the surface energy, which improves paint adhesion and can affect a subsequent laser mark. If the part is going to be printed or bonded, blast first and test the adhesion before production.
FAQ
- Does bead blasting change dimensions?
- It removes 2-5 µm and rounds edges. Usually negligible, significant on fine features.
- Why bead blast before anodizing?
- Clear anodize shows tool marks. A blast gives a uniform matte base.
- Glass bead or aluminum oxide?
- Glass bead for a smooth matte; aluminum oxide cuts rougher and is used as a paint key.
- Can you blast only part of the part?
- Yes, with masking. Masking is manual work and it is priced.
- Will it hide a deep scratch?
- No. It hides tool marks, not damage.
- Does it work on stainless?
- Yes, and it is common before passivation or electropolishing.
- Can it damage a thin part?
- At high pressure on a thin section, yes. The peening can distort it.
- How is the finish controlled?
- By media, pressure, distance and time, checked against an approved sample.
Have a drawing to review?
Send the model, the revision and the quantity. You get a written review of the open items with the price.