Passivation
Stainless steel passivates itself by forming a chromium oxide layer. Machining leaves free iron on the surface, which rusts, and the oxide layer cannot form through it. Passivation removes the iron so the layer can.
Send a drawingWhy a stainless part rusts
Stainless contains chromium, which oxidises instantly and forms a passive layer a few atoms thick. That layer is what makes the metal corrosion resistant — not the bulk alloy.
Machining transfers iron from the tool and leaves embedded particles. That iron rusts in a humid environment, and the rust looks like the stainless itself is failing. It is not: it is contamination.
| Cause | What it looks like | Fix |
|---|---|---|
| Free iron from tooling | Rust spots, especially at edges | Passivation |
| Weld heat tint | Discolouration, low corrosion | Pickling or grinding, then passivate |
| Embedded particles | Pitting at the surface | Electropolishing |
| Chloride attack | Pitting in service | Different alloy (316L) |
Citric versus nitric
Nitric acid is the traditional passivation and is specified by older standards. Citric acid is newer, safer to handle, and performs at least as well on the common 300-series alloys.
Some customer specifications still call out nitric, usually because the specification predates citric. If the drawing says ASTM A967, either is acceptable; if it names a specific acid, follow it.
| Aspect | Citric | Nitric |
|---|---|---|
| Safety | Safer | Corrosive, fume hazard |
| Effectiveness (304/316) | Equal or better | Good |
| Effect on 400-series | Less effective | Better |
| Waste treatment | Simpler | More regulated |
| Common spec | ASTM A967 | ASTM A967 / AMS 2700 |
Verification
Passivation is verified by a test, not by looking at the part. The common ones are a water immersion test, a copper sulphate test for free iron, or a salt spray test for corrosion resistance.
The tests are specified by the customer or the standard. Ask which one applies before the parts are processed, because a failed test means re-processing, not re-machining.
FAQ
- Does passivation change dimensions?
- No. It removes surface contamination, not metal. Electropolishing does remove a few microns.
- Citric or nitric?
- Either, on 304 and 316. Follow the customer’s specification if it names one.
- How is passivation verified?
- A water immersion, copper sulphate or salt spray test — specified by the standard or the customer.
Have a drawing to review?
Send the model, the revision and the quantity. You get a written review of the open items with the price.