Material x process

Brass CNC machining

Brass is the easiest metal to machine and the easiest to get wrong commercially. The machining is trivial; the questions that matter are lead content, dezincification, and whether the part is allowed to be brass at all.

Send a drawing

Why C360 cuts like nothing else

Free-cutting brass C36000 contains about 3% lead, which acts as an internal lubricant and chip breaker. The result is small discontinuous chips, low cutting force, excellent surface finish and tool life measured in tens of thousands of parts.

Speeds of 200-300 m/min are normal, and the limiting factor is usually the part handling, not the cutting. That is why brass turned parts are among the cheapest precision parts made.

GradeLead contentMachinabilityUse
C36000~3%BestGeneral turned and milled parts, dry service
C35300~1.5%Very goodWhere slightly less lead is required
C27450 / C69300<0.1% (lead-free)GoodPotable water, RoHS-sensitive markets
C26000 (cartridge)NoneFairFormed parts, not free machining

Lead, RoHS and drinking water

A part that touches drinking water or falls under RoHS cannot use C360 in many markets. The lead-free alternatives machine well but not as fast, so the price rises by 15-30% for the same geometry.

This is a compliance question, not a machining question, and it has to be settled before the quote. A buyer who specifies C360 for a potable water fitting has a design problem that no machine shop can solve.

Dezincification

In warm, chlorinated or stagnant water, brass can lose zinc from the surface and become porous — dezincification. The part looks fine and then leaks.

Arsenical brass or a dezincification-resistant grade (DZR, such as C35300 or a bronze) is the answer, or a protective plating. Again, a material decision.

Machining notes specific to brass

Soft brass marks easily. Clamping in a serrated jaw leaves a pattern that cannot be polished out of a cosmetic face, so soft jaws or a collet are the default for visible parts.

Fine threads in thin walls collapse under clamping before the thread strips; a support or a thicker wall is cheaper than a repair. And brass burrs on cross-holes smear rather than break, so a light chamfer is usually specified.

IssueCauseFix
Clamp marks on cosmetic facesSerrated jaws on soft brassSoft jaws, collet, or a sacrificial pad
Collapsed thread in thin wallClamping force over a thin sectionSupport, or thicker wall
Smeared burr on cross-holesDuctile chip, no clean breakSpecify a chamfer, use a sharp drill
Stained surface after handlingSkin oils and humidityPack with VCI or lacquer

FAQ

Is C360 safe for drinking water?
Not in many markets. C360 contains about 3% lead. Use a lead-free grade such as C27450 or C69300 for potable water.
Why is lead-free brass more expensive?
It machines 15-30% slower and the material costs more. The difference is real, not a markup.
Can brass be anodized?
No. Brass is plated (nickel, tin, chrome) or lacquered. Anodizing is an aluminum process.

Have a drawing to review?

Send the model, the revision and the quantity. You get a written review of the open items with the price.

Send a drawing →

Privacy policy